Table 2 - Dimensions and Physical Characteristics of Copper Tube: Types K, L, ACR and Gas

Outside Diameter (inches)Tube Type (1)Nominal or Standard Size (inches)Inside Diameter (inches)Wall Thickness (inches)Cross Sectional Area of Bore (sq. inches)Weight of Tube Only, (pounds per linear ft.)Contents of Tube per Linear Foot (cubic feet)
0.375 K 1/4 0.305 0.035 0.073 0.145 0.00051
L 1/4 0.315 0.030 0.078 0.126 0.00054
ACR (D) 3/8 0.315 0.030 0.078 0.126 0.00054
ACR (A) 3/8 0.311 0.032 0.076 0.134 0.00053
GAS 3/8 0.311 0.032 0.076 0.134 0.00053
0.500 K 3/8 0.402 0.049 0.127 0.269 0.00088
L 3/8 0.430 0.035 0.145 0.198 0.00101
ACR (D) 1/2 0.430 0.035 0.145 0.198 0.00101
ACR (A) 1/2 0.436 0.032 0.149 0.182 0.00103
GAS 1/2 0.436 0.032 0.149 0.182 0.00103
0.625 K 1/2 0.527 0.049 0.218 0.344 0.00151
L 1/2 0.545 0.040 0.233 0.285 0.00162
ACR (D) 5/8 0.545 0.040 0.233 0.285 0.00162
ACR (A) 5/8 0.555 0.035 0.242 0.251 0.00168
GAS 5/8 0.555 0.035 0.242 0.251 0.00168
0.750 K 5/8 0.652 0.049 0.334 0.418 0.00232
L 5/8 0.666 0.042 0.348 0.362 0.00242
ACR (D, A) 3/4 0.666 0.042 0.348 0.362 0.00242
ACR (A) 3/4 0.680 0.035 0.363 0.305 0.00252
GAS 3/4 0.680 0.035 0.363 0.305 0.00252
0.875 K 3/4 0.745 0.065 0.436 0.641 0.00303
L 3/4 0.785 0.045 0.484 0.455 0.00336
GAS 7/8 0.785 0.045 0.484 0.455 0.00336
ACR (D, A) 7/8 0.785 0.045 0.484 0.455 0.00336
1.125 K 1 0.995 0.065 0.778 0.839 0.0054
L 1 1.025 0.050 0.825 0.655 0.00573
GAS 1 1/8 1.025 0.050 0.825 0.655 0.00573
ACR (D, A) 1 1/8 1.025 0.050 0.825 0.655 0.00573
1.375 K 1 1/4 1.245 0.065 1.220 1.04 0.00847
L 1 1/4 1.265 0.055 1.260 0.884 0.00875
ACR (D,A) 1 3/8 1.265 0.055 1.260 0.884 0.00875
1.625 K 1 1/2 1.481 0.072 1.720 1.36 0.0119
L 1 1/2 1.505 0.060 1.780 1.14 0.0124
ACR (D,A) 1 5/8 1.505 0.060 1.780 1.14 0.0124
2.125 K 2 1.959 0.083 3.010 2.06 0.0209
L 2 1.985 0.070 3.090 1.75 0.0215
ACR (D) 2 1/8 1.985 0.070 3.090 1.75 0.0215
2.625 K 2 1/4 2.435 0.095 4.660 2.93 0.0324
L 2 1/2 2.465 0.080 4.770 2.48 0.0331
ACR (D) 2 5/8 2.465 0.080 4.770 2.48 0.0331
3.125 K 3 2.907 0.109 6.640 4 0.0461
L 3 2.945 0.090 6.810 3.33 0.0473
ACR (D) 3 1/8 2.945 0.090 6.810 3.33 0.0473
Notes:
1: D= Drawn temper, A= Annealed temper